Charpy impact values of Precipitation hardened SS 17-4PH

  • 1.  Charpy impact values of Precipitation hardened SS 17-4PH

    Bangalore Admin
    Posted 07-27-2020 08:37
    Continuing my problem with the charpy values of Investment cast 17-4PH, I want to clarify that the product has been heat treated as follows: Solutionised at 1080 deg C( water quenched) followed by double age hardening as per H1150 to get a hardness of 30-33HRc.

    ------------------------------
    Dilip Raman
    Consultant- Metallurgy
    Bangalore
    (91)9980073171
    ------------------------------


  • 2.  RE: Charpy impact values of Precipitation hardened SS 17-4PH

    Posted 07-28-2020 12:27
    How is the fractured surface look like? is it brittle or ductile? If it is brittle then I suspect you have copper segregation along the grain boundaries. Can be identified by SEM probe analysis in Lab.

    ------------------------------