  • 1.  Steel alloy

    Posted 03-09-2025 09:27
    Does anyone have info on analysis and availability of alloy 1020 steel in bars?
    ASM Education Summer Sale


  • 2.  RE: Steel alloy

    Posted 03-10-2025 08:34

    What shape and quality of bars are you seeking?  1020 comes in a merchant grade covered under ASTM A575 or SBQ to various specifications such as ASTM A576.

     

    Merchant 1020 according to ASTM A575 Table 1 is M1020 – C: 0.17-0.24, Mn: 0.25-0.60, P:  0.04 max, S: 0.05 max.

    SBQ 1020 (G10200) according to ASTM A576 Table 1 is C: 0.18-0.23, Mn: 0.30-0.60, P:  0.040 max, S: 0.050 max

     

    Daniel Wells

    Quality Manager

    Gerdau – Wilton Mill

     

    1500 West 3rd Street

    Wilton, IA 52778

    Office: (563) 279-1238

    Cell: 608-851-0077

    Daniel.Wells1@gerdau.com

     

    This message may include restricted, legally privileged, and/or confidential information. If you received this message by mistake please delete it immediately and inform us about it. This message will be considered as originated from Gerdau or its subsidiaries only when formally confirmed by its officers authorized for that.

    Este mensaje puede contener informaciones de uso restringido y/o legalmente protegido. Si usted ha recibido este mensaje por error, por favor eliminelo e informe de tal situación al remitente. Este mensaje solamente será considerado como proveniente de Gerdau o de sus subsidiarias cuando sea confirmado formalmente a través de los representantes legales debidamente autorizados para tal fin.


    This content is Public.




    ASM Education Summer Sale